The problems encountered in casting titanium in dentistry have not been completely resolved. The Procera system forms crowns by means of a combination of spark-erosion and milling. The accuracy of fit was examined before and after ceramic veneering both in vitro and in vivo. Before veneering, on conical surfaces space widths were approximately 53-mu-m in vitro and 69-mu-m in vivo. At shoulders and occlusal surfaces, spaces of about 430-mu-m were measured in vitro and of about 500-mu-m were measured in vivo. After ceramic veneering, slight increases in space widths could be observed. The metal-ceramic compound was tested by the 3-point bending test (DIN) and the bending test (ISO). The DIN test was satisfactory, but not the ISO test. It is concluded that titanium crowns processed by the Procera System are suitable for clinical usage, if the space widths at shoulders and the occlusal surface and the special requirements of tooth preparation are taken into account.